Investigation of influence of silicon carbide fractional composition on thermal conductivity of composite material based on aluminium alloy

Nyafkin A.N., Loshinin U.V., Kurbatkina E.I., Kosolapov D.V.
Nyafkin A.N., Loshinin U.V., Kurbatkina E.I., Kosolapov D.V. Investigation of influence of silicon carbide fractional composition on thermal conductivity of composite material based on aluminium alloy // Proceedings of VIAM. 2019. No. 11. DOI: 10.18577/2307-6046-2019-0-11-53-59. URL: https://viam-works.ru/en/journal/2019/11/6
Keywords
vacuum compression impregnation, highly filled metal composite material, aluminum alloy, silicon carbide, thermal conductivity, thermophysical properties.
Abstract

In work the metal composite material on the basis of the aluminum foundry alloy of the AK7 brand containing 65±1 vol. % silicon carbide was developed and investigated and obtained using the technology of vacuum-compression impregnation. Porous billets with different fractional composition of silicon carbide were obtained by cold compaction followed by impregnation with aluminum alloy melt. Samples were made for the study of thermal conductivity and heat capacity of a composite material with different fractional composition of silicon carbide. Measurements of the characteristics of the thermophysical properties – heat capacity, thermal conductivity and thermal diffusivity in the temperature range from -100 to +400°C – of a composite material with different fractional composition of silicon carbide were carried out.

Reference list
  1. Kablov E.N., Shchetanov B.V., Shavnev A.A., Nyafkin A.N. i dr. Povysheniye nadezhnosti silovykh IGBT-moduley s pomoshchyu vysokonapolnennogo MKM sistemy Al–SiC [Increase of reliability of power IGBT-modulus by means of high filled metal matrix composite of Al–SiC system] // Aviacionnye materialy i tehnologii. 2010. №4. S. 3–6.
  2. Kablov E.N. Innovacionnye razrabotki FGUP «VIAM» GNC RF po realizacii «Strategicheskih napravlenij razvitiya materialov i tehnologij ih pererabotki na period do 2030 goda» [Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030»] // Aviacionnye materialy i tehnologii. 2015. №1 (34). S. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
  3. Kablov E.N., Shchetanov B.V., Shavnev A.A., Nyafkin A.N. i dr. Svoystva i primeneniye vysokonapolnennogo metallomatrichnogo kompozitsionnogo materiala Al–SiC [Properties and application of a highly filled metal matrix composite material Al – SiC] // Tekhnologiya mashinostroyeniya. 2011. №3 (105). S. 5–7.
  4. Kablov E.N., Shchetanov B.V., Grashhenkov D.V., Shavnev A.A., Nyafkin A.N. Metallomatrichnye kompozicionnye materialy na osnove Al–SiC [Metalmatrix composite materials on the basis of Al–SiC] // Aviacionnye materialy i tehnologii. 2012. №S. S. 373–380.
  5. Kablov E.N., Chibirkin V.V., Vdovin S.M. Izgotovlenie, svojstva i primenenie teplootvodyashchih osnovanij iz MMK Al–SiC v silovoj elektronike i preobrazovatelnoj tehnike [Manufacturing, properties and application of the heat-removing bases from Al–SiC MMK in power electronics and converting equipment] // Aviacionnye materialy i tehnologii. 2012. №2. S. 20–22.
  6. Nyafkin A.N., Grishina O.I., Shavnev A.A., Loshchinin Yu.V., Pakhomkin S.I. Issledovaniye vliyaniya sostava geterogennykh sistem s vysokim soderzhaniyem karbidnoy fazy na teplofizicheskiye svoystva [The influence of composition of heterogeneous systems with a high of the carbide phase on thermo-physical properties] // Aviacionnye materialy i tehnologii. 2014. №S6. S. 28–34. DOI: 10.18577/2071-9140-2014-0-s6-28-34.
  7. Goncharenko E.S., Trapeznikov A.V., Ogorodov D.V. Litejnye alyuminievye splavy (k 100-letiyu so dnya rozhdeniya M.B. Altmana) [Aluminium casting alloys] // Trudy VIAM: elektron. nauch.-tehnich. zhurn. 2014. №4. St. 02. Available at: http://www.viam-works.ru (accessed: October 03, 2019). DOI: 10.18577/2307-6046-2014-0-4-2-2.
  8. Ustroystvo dlya polucheniya izdeliya iz metallomatrichnogo kompozitsionnogo materiala: pat. 110310 Ros. Federatsiya [A device for producing products from a metal matrix composite material: pat. 110310 Rus. Federation]; zayavl. 31.05.11; opubl. 20.11.11.
  9. Sposob polucheniya izdeliya iz kompozitsionnogo materiala: pat. 2448808 Ros. Federatsiya [The method of obtaining products from composite material: pat. 2448808 Rus. Federation]; zayavl. 05.10.10; opubl. 27.04.12.
  10. Parker W.J., Jenkins R.J., Butler S.R., Abbott G.L. Rash method of determining thermal diffusivity, heat capacity and thermal conductivity // Journal of Applied Physics. 1961. No. 32. P. 1679–1684.
  11. ASTM E 1461-01. Standard test method for thermal diffusivity by the flash method. 2001. P. 11–13.
  12. Chekhovskoy V.Ya., Peletskiy V.E. Teplofizicheskiye svoystva zharoprochnogo splava na nikelevoy osnove KhN55VMTKYu (EI929) [Thermophysical properties of heat-resistant nickel-based alloy KhN55VMTKYu (EI929)] // Teplofizika vysokikh temperatur. 2005. T. 43. №1. S. 51–56.
  13. Xue J., Taylor R. An evaluation of specific heat measurement methods using the laser flash technique // International Journal of Thermophysics. 1993. Vol. 14. No. 2. P. 313–320.
  14. GSSSD 65–84. Tablitsy standartnykh spravochnykh dannykh. Korund sinteticheskiy. Izobarnaya teployemkost v diapazone temperatur 4–2300 K [State Standard Reference Data Service 65–84. Tables of standard reference data. Synthetic corundum. Isobaric heat capacity in the temperature range 4–2300 K]. M.: Izd-vo standartov, 1985. 6 s.
  15. Gurvich M.E., Larikov L.N., Nozar A.I. Optimizatsiya metoda skaniruyushchego adiabaticheskogo kalorimetra [Optimization of the method of scanning adiabatic calorimeter] // Inzhenerno-fizicheskiy zhurnal. 1981. T. 41. №7. S. 129–135.
  16. GOST 18898–89 (ISO 2738–87). Izdeliya poroshkovyye. Metody opredeleniya plotnosti, soderzhaniya masla i poristosti [State Standard 18898–89 (ISO 2738–87). Powder products. Methods for determination of density, oil content and porosity]. M.: Izd-vo standartov, 1990. 10 s.
  17. Beletskiy V.M., Krivov G.A. Alyuminiyevyye splavy. Sostav, svoystva, tekhnologii, primeneniye: spravochnik / pod obshch. red. I.N. Fridlyandera [Aluminum alloys. Composition, properties, technologies, application: reference book / gen. ed. I.N. Friedlander]. Kiev: Komintekh, 2005. 365 s.