Development of combined heat-resistant coatings for parts made of natural-composite material based on niobium

Kashin D.S., Stekhov P.A.
Kashin D.S., Stekhov P.A. Development of combined heat-resistant coatings for parts made of natural-composite material based on niobium // Proceedings of VIAM. 2017. No. 6. DOI: 10.18577/2307-6046-2017-0-6-4-4. URL: https://viam-works.ru/en/journal/2017/6/4
Keywords
heat resistant coatings, ion-plasma coatings, high-temperature gas corrosion, niobium based heat-proof alloy, barrier layer, siliconizing.
Abstract

Researches of isothermal heat resistance of samples from natural-composite material are based on niobium for GTE parts with heat-resistant coatings at a temperature of 1350°C on the basis of tests of 30 hours. Tests on the cyclic heat resistance of samples with a combined coating at a temperature of 500⇄1300°C with air cooling up to 500°C have been carried out. Investigations of the microstructures of the coatings in their original form and after tests on the heat resistance of samples from a naturally-composite material based on niobium with complex coatings were carried out. The coating of the Si+(Fe–Cr–Al–Y)+Si system has a higher crack resistance than the diffusion heat-resistant coating. Combined heat-resistant coating provides protection of parts from natural-composite material based on niobium at operating temperatures up to 1350°C, and preserves protective properties under thermal cycling conditions.

Reference list
  1. Litye lopatki gazoturbinnyh dvigatelej: splavy, tehnologii, pokrytiya / pod obshh. red. E.N. Kablova. 2-e izd. [Cast blades of gas turbine engines: alloys, technologies, coverings / gen. ed. by E.N. Kablov, 2nd ed.]. M.: Nauka, 2006. 632 s.
  2. Kablov E.N., Petrushin N.V., Sidorov V.V. Rhenium in the thermally stable nickel alloys for single‐crystal blades of gas‐turbine engines // 7th International Symposium on Technetium and Rhenium Science and Utilization. 2011. P. 1–7.
  3. Matveev P.V., Budinovskij S.A., Muboyadzhyan S.A., Kosmin A.A. Zashhitnye zharostojkie pokrytiya dlya splavov na osnove intermetallidov nikelya [High-temperature coatings for intermetallic nickel-based alloys] //Aviacionnye materialy i tehnologii. 2013. №2. S. 12–15.
  4. Kablov E.N., Petrushin N.V., Svetlov I.L., Demonis I.M. Nikelevye litejnye zharoprochnye splavy novogo pokoleniya [Nickel foundry heat resisting alloys of new generation] // Aviacionnye materialy i tehnologii. 2012. №S. C. 36–52.
  5. Zaharova G.V., Popov I.A., Zhorova L.P., Fedin B.V. Niobij i ego splavy [Niobium and its alloys]. M.: Gos. nauch.-tehn. izd-vo lit-ry po chernoj i cvetnoj metallurgii, 1961. 196 s.
  6. Svetlov I.L. Vysokotemperaturnye Nb–Si kompozity [High-temperature Nb–Si composites] // Materialovedenie. 2010. №9–10. S. 18–38.
  7. Kablov E.N., Muboyadzhyan S.A. Heat-resistant coatings for the high-pressure turbine blades of promising gtes // Russian metallurgy (Metally). 2012. No. 1. P. 1–7.
  8. Kablov E.N., Muboyadzhyan S.A. Zharostojkie i teplozashhitnye pokrytiya dlya lopatok turbiny vysokogo davleniya perspektivnyh GTD [Heat resisting and heat-protective coverings for turbine blades of high pressure of perspective GTE] // Aviacionnye materialy i tehnologii. 2012. №S. S. 60–70.
  9. Hayashi S., Takagi S., Yamagata R., Narita T., Ukai S. Formation of Exclusive Al2O3 Scale on Nb and Nb-Rich Alloys by Two-Step Oxygen-Aluminum Diffusion Process // Oxidation of Metals. 2012. No. 78. P. 167–178.
  10. Sosnovskij L.A., Kaplina G.S., Astahova Zh.A., Korol E.A. Kompleksnye silicidnye pokrytiya na niobii [Complex silicide coverings on niobium] // Vysokotemperaturnaya zashhita materialov. L.: Nauka, 1981. S. 83–86.
  11. Kablov E.N., Muboyadzhyan S.A., Budinovskij S.A., Lucenko A.N. Ionno-plazmennye zashhitnye pokrytiya dlya lopatok gazoturbinnyh dvigatelej [Ion-plasma protecting covers for blades of gas turbine engines] // Metally. 2007. №5. S. 23–34.
  12. Streiff R. Protection of materials by advanced high temperature Coatings // Journal de physique IV. 1993. Vol. 3. No. 111. P. 17–41.
  13. Fukumoto M., Matsumura Y., Hayashi S. et al. Coatings of Nb-based Alloy by Cr and/or Al Pack Cementations and Its Oxidation Bahavior in Air at 1273–1473 K // Materials Transactions. 2003. Vol. 44. No. 4. P. 731–735.
  14. Novak M., Levi C. Oxidation and Volatilization of Silicide Coatings for Refractory Niobium Alloys // Proceedings of IMECE. Seattle, 2007. P. 3–5.
  15. Tsirlin M.S., Kasatkin A.V., Byalobzheskii A.V. An oxidation-resistant silicide coating for niobium alloys // Poroshkovaya metallurgiya. 1978. No. 12. P. 31–34.
  16. Oxidation resistant coating for Niobium – based silicide Composites: pat. 6521356 US; publ. 18.02.03.
  17. Stupik D., Donovn M.M., Barronj A.R. et al. The interfacial mixing of silicon coatings on niobium metal: a comparative study // Thin Solid Films. 1992. No. 207. P. 138–143.
  18. Kablov E.N. Innovacionnye razrabotki FGUP «VIAM» GNC RF po realizacii «Strategicheskih napravlenij razvitiya materialov i tehnologij ih pererabotki na period do 2030 goda» [Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030»] // Aviacionnye materialy i tehnologii. 2015. №1 (34). S. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.