Investigation of diffusion of alloying elements during thermal cycling of multilayer composite material made of chrome and carbon steels

Khudnev A.A., Plokhikh A.I., Dvoretskov R.M., Schetanov B. V.
Khudnev A.A., Plokhikh A.I., Dvoretskov R.M., Schetanov B. V. Investigation of diffusion of alloying elements during thermal cycling of multilayer composite material made of chrome and carbon steels // Proceedings of VIAM. 2021. No. 4. DOI: 10.18577/2307-6046-2021-0-4-74-91. URL: https://viam-works.ru/en/journal/2021/4/6
Keywords
layered metal composite material, steel U8, steel 08H18, diffusion, microstructure, hot rolling.
Abstract

In this work the effect of five cycles of heating to a temperature of 1000 °C and three cycles of heating to a temperature of 1100 °C on the structure of multilayered composite material consisted of 100 alternating layers of 08H18 and U8 steels was investigated via the methods of microstructural analysis. It is shown that already in the initial state after rolling there was a redistribution of carbon between the layers of the material. Thermal cycling led to a partial redistribution of chromium in the material, a change in the structure and thickness of the layers.

Reference list
  1. Kablov E.N. The strategic directions of development of materials and technologies of their processing for the period to 2030. Aviacionnye materialy i tehnologii, 2012, no. S, pp. 7–17.
  2. Kashin D.S., Dergacheva P.E., Stekhov P.A. Heat resistant slurry coatings (review). Trudy VIAM, 2018, no. 5 (65), paper no. 08. Available at: http://www.viam-works.ru (accessed: December 17, 2020). DOI: 10.18577/2307-6046-2018-0-5-64-75.
  3. Trofimenko N.N., Efimochkin I.Yu., Bolshakova A.N. Problems of creation and prospects for the use of heat-resistant high-entropy alloys. Aviacionnye materialy i tehnologii, 2018, no. 2 (51), pp. 3–8. DOI: 10.18577/2071-9140-2018-0-2-3-8.
  4. Grashchenkov D.V., Efimochkin I.Yu., Bolshakova A.N. High-temperature metal-matrix composite materials reinforced with particles and fibers of refractory compounds. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 318–328. DOI: 10.18577/2071-9140-2017-0-S-318-328.
  5. Kablov E.N. New generation materials – the basis of innovation, technological leadership and national security of Russia. Intellekt & Tekhnologii, 2016, no. 2, pp. 41–46.
  6. Kablov E.N. New generation materials and digital technologies for their processing. Bulletin of the Vestnik Rossiyskoy akademii nauk, 2020, vol. 90, no. 4, pp. 331–334.
  7. Kablov E.N., Antipov V.V., Senatorova O.G., Lukina N.F. A new class of laminated aluminum-glass-fiber-reinforced plastics based on an aluminum-lithium alloy 1441 with a reduced density. Vestnik MGTU im. N.E. Bauman, ser.: Mechanical engineering, 2011, no. SP2, pp. 174–183.
  8. Kablov E.N., Antipov V.V., Klochkova Yu.Yu. Aluminum-lithium alloys of a new generation and layered aluminum-glass-fiber-reinforced plastics based on them. Tsvetnye metally, 2016, no. 8, pp. 86–91.
  9. Schmiedt A., Luecker L., Kolesnikov A., Plokhikh A.I., Walther F. Production- and microstructure-based fatigue assessment of metallic AISI 304/430 multilayer materials produced by hot pack rolling. Materialpruefung, 2017, vol. 59 (2), pp. 123-129.
  10. Karpov M.I., Vnukov V.I., Medved N.V. et al. Possibilities of the vacuum rolling method as a method of obtaining multilayer composites with nanometric thicknesses of layers. Materialovedenie, 2004, no. 1, pp. 48–53.
  11. Kobelev AG, Lysak VI, Chernyshev VN et al. Production of layered composite materials. Moscow: Intermet-Inzhiniring, 2002, 496 p.
  12. Batiyenkov R.V., Bolshakova A.N., Efimochkin I.Yu. The problem of low-temperature plasticity of molybdenum and alloys based on it (review). Trudy VIAM, 2018, no. 3 (63), paper no. 02. Available at: http://www.viam-works.ru (accessed: December 11, 2020). DOI: 10.18577/2307-6046-2018-0-3-12-17.
  13. Chuvildeev V.N., Shchavleva A.V., Nokhrin A.V. et al. Influence of grain size and structural state of grain boundaries on the parameters of low-temperature and high-speed superplasticity of nano- and microcrystalline alloys. Fizika tverdogo tela, 2010, vol. 52, no. 5, pp. 1026–1033.
  14. Korzhov V.P., Karpov M.I., Prokhorov D.V. Multilayer structure and high-temperature strength of heat-resistant materials based on compounds of niobium with aluminum and silicon obtained from composites Nb–Al and Nb–Si. Fizika i tekhnika vysokikh davleniy, 2013, vol. 23, no. 1, pp. 99–107.
  15. Firstov S.A., Karpov M.I., Korzhov V.P. et al. The structure and properties of a layered composite made of a high-entropy alloy with carbide and intermetallic hardening. Izvestiya Rossiyskoy akademii nauk, ser.: Physical, 2015, vol. 79, no. 9, pp. 1267–1267.
  16. Karpov M.I., Korzhov V.P., Kiiko V.M. et al. Influence of heat treatment under pressure on the structure of layered composites Ni/Al. Perspektivnyye materialy, 2011, no. S13, pp. 704–712.
  17. Kolesnikov A.G., Plokhikh A.I., Komisarchuk Yu.S., Mikhaltsevich I.Yu. Investigation of the peculiarities of the formation of a submicro- and nanoscale structure in multilayer materials by the hot rolling method. Metallovedeniye i termicheskaya obrabotka metallov, 2010, no. 6, pp. 44–49.
  18. Plokhikh A.I., Vlasova D.V., Khovova O.M., Polyansky V.M. Investigation of the influence of diffusion mobility of alloying elements on the stability of the structure of multilayer metallic materials. Nauka i obrazovanie, 2011, no. 11. Available at: http://technomag.edu.ru/doc/262116.html (accessed: December 15, 2020).
  19. Arzamasov B.N., Makarova V.I., Mukhin G.G. et al. Materials Science. 8th ed. Moscow: MSTU im. N.E.Bauman, 2008, 648 p.
  20. Gasik M.I., Lyakishev N.P. Theory and technology of electrometallurgy of ferroalloys: Textbook. Moscow: Intermet-Inzhiniring, 1999, 764 p.
  21. Blanter M.E. Metallurgy and heat treatment. Moscow: Mashgiz, 1963, 416 p.
  22. Lee C. G., Iijima Y., Hiratani T., Hirano K. Diffusion of chromium in α-iron. Materials Transactions, JIM, 1990, vol. 31, no. 4, pp. 255–261.
  23. Blanter M.E. Phase transformations during heat treatment of steel. Moscow: Metallurgizdat, 1962, 268 p.
  24. Tabatchikova T.I., Plokhikh A.I., Yakovlev I.L., Klyueva S.Yu. Structure and properties of multilayer material on the basis of steels obtained by hot batch rolling. Fizika metallov i metallovedenie, 2013, vol. 114, no. 7, pp. 633–647.
  25. Vlasova DV, Plokhikh AI, Semenov M.Yu. et al. Diffusion in multilayer materials based on carbon and alloy steels obtained by hot batch rolling. Metallurg, 2018, no. 5, pp. 33–38.
  26. Kintsel A.B., Franks R. High-chromium stainless and heat-resistant steels. Moscow: Metallurgizdat, 1945.473 p.
  27. Plokhikh A.I., Chan Yu., Karpukhin S.D. Investigation of the influence of interlayer diffusion carbon redistribution on the impact toughness of multilayer materials. Izvestiya Volgogradskogo gosudarstvennogo tekhnicheskogo universiteta, 2015, no. 8, pp. 86–91.
  28. Heat treatment in mechanical engineering: a reference book. Ed. Yu.M. Lakhtin, A.G. Rakhstadt. Moscow: Mashinostroenie, 1980, 783 p.
  29. Sozykina A.S., Okishev K.Yu. Phase equilibria and transformations in high-chromium iron alloys: textbook. Chelyabinsk: IC SUSU, 2019, 40 p.
  30. Bungardt K., Kunze E., Horn E. Untersuchungen über den Aufbau des Systems Eisen – Chrom – Kohlenstoff. Archiv für das Eisenhüttenwesen, 1958, vol. 29, no. 3, pp. 193–203.
  31. Sozykina A.S. Modeling of transformations during austenitization and quenching and forecasting the hardness of high-chromium steels and cast irons on the basis of thermodynamic and kinetic calculations: thesis, Cand. Sc. (Tech.). Chelyabinsk: SUSU, 2018, 153 p.